SharonR (not verified)

I have not been able to dye this week either. I am working on the reading and color exercises.  I also went back to the color chips from last week-I made a few mistakes. I have been weighing my yarn and attempting to use the niddy noddy. I am not sure if I am tying the knots right. How far apart should they be or how many to secure the yarn? Also, I have not been able to locate the sodium hexametaphosphate-I will have to order it. Is there anything else I can use?

Mary Rios (not verified)

Sharon, initially i was trying to make small skeins on a skein winder set to less than 1m. that was slow and messy - Cathie suggested taking a book, and wrapping the book. I'm using 8/2 silk and the size book i use, take about 62 wraps. It goes fast and works.

SharonR (not verified)

Yes, I am new to working with yarn (other than knitting). I am interested in making the silk samples, but do want to learn to dye the yarn. I do have a filter so I will try that with the water. I plan to catch up with everything this weekend so I am not further behind. It is taking me a little time to understand the Munsell notation-that is why I had to go back and reassign numbers for last weeks assignment.

pjdoney (not verified)

1)  Dry skein weigh - soak in water

2)  Make 1% stock solution

3)  Ready "chemical" water (pH 4.5, A. Set, Na Acetate, Glauber's NaCl)

4)  Do the math for mL for individual dye colors

5)  Prepare dye bath

6)  Process:

     Add damp skeins (10 min)

     Add measured dye stock  (10 min)

     Heat gradually to 95 C (203 F - I have altitude issues)

     Hold at 95 C approximately 1 hr, lift skeins occasionally

     Cool down room temp

     Remove skein, rinse, spin, hang to dry

 

 

 

pjdoney (not verified)

I know that there isn't table salt, only Glauber's.  I was racking my brain for subscripts so I wrote out the chemical formula for regular salt for short hand.  I was primarily writing for a general process as opposed to the trial dyeing runs. 

And yes, 100 mL of olive! 

They did indeed leave me behind for their honeymoon but now I get to have the dye studio.  I think that is honeymoon enough for me.  : )

pjdoney (not verified)

Rocky Mountain Dyeing Process

1)  Dry skein weigh - soak in water

2)  Make 1% stock solution of olive green (58 mL gold, 29 mL turquoise, 13 mL magenta)

3)  Ready "chemical" water (pH 4.5,  1/4 tsp/ 2.5L A. Set, 1/4 tsp Na Acetate/ 5L, 2 gr/ L Glauber)

4)  Process:

     Add damp skeins (10 min)

     Add 2.25 mL Olive dye  (10 min)

     Heat gradually to 95 C (203 F - I have altitude issues)

     Hold at 95 C approximately 1 hr, lift skeins occasionally

     Cool down room temp

     Remove skein, rinse, spin, hang to dry

pjdoney (not verified)

Yes, the 2.25 mL of dye stock is for a 5 gram wool skein dyed at 0.45% DOS.

I will avoid using the term "chemical water".  Does dye bath to you mean the water, acetic acid, sodium acetate, and Glauber or the preceeding four items AND dye stock?  I'm probably still fuzzy headed from the wedding - I think I've been reading interpetations for both.

Definitely feeling overwhelmed with the system not working properly.  Today I have to do a lot of other non-dyeing tasks so I hope to get my 5 L of dye bath made again and do (hopefully) one round of dyeing.

pjdoney (not verified)

My pH looked correct before starting (4.5 or 4.6) and at the end of the dye session is now 5.0.  My guess is this won't exhaust very well either.

pjdoney (not verified)

My results look to be about the same old, same old color.  I think a little more dye did exhaust this time but there's still a lot of red in the water.  My guess is that in trying to get the high temp that water surrounding the jar would splash into the jar with skein and dye.  Knowing that my water has a pH of 5.3, I am assuming that is the culprit for the raising of my pH level to 5.0 from 4.5/ 4.6.

I could try putting aluminum foil over the top of the dye jar once the water bath gets more active.  I would prefer waiting to do that until I put the lid on the pot because of fussing but that might not be an option. 

I can send you a picture but honestly, you've already seen very similar results.  Do you want me to post on the spreadsheet?

pjdoney (not verified)

Share the misery....before and after pH pictures:

 

Made my new dye bath using 5 L water, 1/2 tsp A. Set, 1/4 tsp Sodium acetate, and 10 gr Glauber salt.  pH was lowered to approx. 4.5 using acetic acid.  Soaked 5 gr skein in water, then soaked in dye bath (10 min), removed skein, put 2.25 mL Olive Green in jar and replaced skein and let it sit (10 min).  In just over an hour temp was raised from 19 C to 94 C with a dwell time of 1 hour (dunking every few minutes).  Cool down of several hours, rinse, etc.

Jeff and I are wondering about making an e-collar out of aluminum foil so I can dunk but hopefully keep out lively water splashes.  That would also allow for me to monitor its temp more easily.